Continuing Folio E.02's concrete placement, E.09's crack healing, and E.11's continuum stiffness: an illustrative fracture-mechanics study coupling Hillerborg's fictitious crack model, Bažant's Type II Size Effect Law, and Bažant–Kazemi regression for initial fracture energy and process-zone length across laboratory beams and deep concrete girders.
Why it matters
Compare tearing a small notched strip of heavy woven cardboard against tearing a wide poster board made of the same card stock. Along the notch tip, loose paper fibers fray and bridge across a finger-width zone about 20 mm wide. On a 30 mm narrow strip, that frayed zone spans nearly the whole remaining ligament, so you feel the strip pull evenly before parting. On a 1,000 mm wide sheet, the same 20 mm frayed zone sits like a tiny pinprick at the notch tip while elastic tension across the broad sheet concentrates energy right into that tip, unzipping the sheet at far lower average stress. This analogy stops where three-dimensional coarse-aggregate interlock and compressive shear friction replace pure tensile fiber tearing.
Conceptual Vision Plate E.15-V (Imagining What It Would Look Like) · Artistic laboratory view imagining geometrically similar notched concrete beams across three structural depths. Governing equations and strength-scaling bounds are kept intact in deterministic Plate E.15-A and the offline verifier below.
About this illustrationThis AI-generated illustration is imagining what the concept would look like: an artistic impression, not a measured structure or specification. Exact geometry, specifications and governing equations are kept strictly intact with zero artistic interpretation in deterministic Plate E.15-A and Plate E.15-B below.Sinopsis Ejecutiva en Español · Folio E.15
Actos I y II — Historia, ley gobernante e intuición cotidiana:Fractura Cuasi-Frágil en Concreto, Ley de Efecto de Tamaño de Bažant y Zona de Proceso — Continuación de los Folios E.02, E.09 y E.11: estudio ilustrativo de mecánica de fractura que acopla la grieta ficticia de Hillerborg, la ley de tamaño Tipo II de Bažant σ_N = B f'_t / √(1 + D / D_0) y la regresión de Bažant–Kazemi para G_f y c_f. Este monográfico interactivo verifica la ley gobernante σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0). Por qué importa en la vida real: Igual que una muesca en cartón ancho concentra la tensión en una franja pequeña de fibras sueltas, una viga profunda de concreto falla a menor esfuerzo nominal que una probeta pequeña del mismo colado.
En Palabras Sencillas (Explicación Accesible): En palabras sencillas, el concreto guarda un colchón de resistencia justo delante de la punta de una grieta. Antes de partirse del todo, piedras ásperas y microfisuras puentean el corte y cargan parte del tirón. En una viga pequeña de laboratorio, esa zona puenteada abarca casi todo el peralte y la sección trabaja cerca de su límite plástico. En una trabe profunda de puente o presa, la zona puenteada conserva casi el mismo espesor físico mientras la pieza crece mucho, concentrando la energía elástica en la muesca.
Mecanismo Técnico, Fuerzas en Competencia y Umbral Crítico: En el modelo de Bažant (1984, DOI 10.1061/(ASCE)0733-9399(1984)110:4(518)) y Hillerborg et al. (1976, DOI 10.1016/0008-8846(76)90007-7), la resistencia nominal de vigas entalladas Tipo II sigue σ_N(D) = B f'_t / √(1 + D / D_0) con número de fragilidad β_B = D / D_0 y pendiente s = −β_B / [2(1 + β_B)]. Con la calibración ilustrativa B f'_t = 4.20 MPa, D_0 = 220.0 mm, E' = 34.0 GPa, f'_t = 3.20 MPa, g(α_0) = 1.12 y g'(α_0) = 3.80, una viga de 100 mm alcanza σ_N = 3.482 MPa (82.9%), una de 400 mm baja a 2.502 MPa (59.6%, β_B = 1.818, s = −0.323) y una trabe de 2,000 mm desciende a 1.322 MPa (31.5%, s = −0.450), frente a 4.20 MPa con el defecto plástico (3.177× mayor). La regresión de Bažant–Kazemi (1990, DOI 10.1007/BF00047063) recupera G_f = 127.84 N/m, c_f = 64.84 mm y l_ch = 424.5 mm. Esta hipótesis de nivel T1–T2 se refuta en vigas sin entalla Tipo I (Bažant y Yu 2009, DOI 10.1061/(ASCE)0733-9399(2009)135:2(78)), elementos con estribos o fibras densas o piezas donde D se aproxima al tamaño del agregado (Qin et al. 2024, DOI 10.1016/j.tafmec.2024.104649).
Acto III — Laboratorio interactivo: los deslizadores en tiempo real y las cuatro lentes del observatorio (superficie 3D, retrato de fase, listón de conservación y radar polar) permiten explorar los umbrales críticos directamente en el navegador.
Actos IV y V — Descubrimiento y fuentes: la narrativa completa y las fuentes primarias siguen abajo (en inglés). Investigación científica y educativa abierta, no consejo médico.
Act I — Cool Fact & Human Story: Why Small Concrete Beams Test Stronger Than Deep Bridge Girders
In 1976, Swedish structural engineer Arne Hillerborg stood before a puzzling gap in how concrete breaks. A small notched concrete beam cast for a university laboratory bench routinely carried higher nominal stress than a geometrically identical beam poured ten times deeper for a bridge pier or dam spillway. Classical plastic strength rules treated material strength as a fixed number independent of member height, while classical brittle fracture predicted a steep drop in strength as beam depth grew. Neither picture matched real concrete structures. Hillerborg and his colleagues Mikael Modéer and Per-Erik Petersson proposed that concrete ahead of a crack tip does not snap cleanly like window glass. Instead, microcracks and rough stone aggregates share tensile stress across a finite softening zone before splitting apart. Explaining how that process zone sets structural brittleness governs safe scaling from laboratory test benches to full civil spans.
In Plain Words · Extra-Easy Explanation
In plain words, concrete carries a hidden cushion ahead of a growing crack. Before a notch opens all the way, rough stones and tiny microcracks bridge the gap and hold part of the load. In a small bench beam, that bridged zone spans most of the height. The whole cross section shares the pull and fails near its plastic strength. In a deep bridge girder or dam wall, the bridged zone stays about the same size while the girder grows much taller. Now the cushion sits in a thin strip near the notch tip. Elastic energy concentrates right ahead of the crack. Standard small cylinders miss this drop in resistance. As a result, a two-meter girder splits at a lower average stress than a small beam from the same batch, even with matching notch proportions.
In 1984, Zdeněk P. Bažant united those two limits—small-scale plastic strength and large-scale Linear Elastic Fracture Mechanics (LEFM, introduced by Alan Arnold Griffith in 1921, DOI 10.1098/rsta.1921.0006[Scite ↗]) in a single asymptotic matching law known as the Type II Size Effect Law (Journal of Engineering Mechanics, DOI 10.1061/(ASCE)0733-9399(1984)110:4(518)[Scite ↗]). Bažant scaled nominal failure stress using structural depth D, transitional size D_0, and small-scale plastic intercept B f'_t so that small members approach plastic yield while deep members approach square-root fracture scaling. Six years later, Bažant and Mohammad T. Kazemi (1990, DOI 10.1007/BF00047063[Scite ↗]) showed that plotting inverse squared strength against depth turns the curve into a line whose slope and intercept extract initial Mode I fracture energy G_f and effective fracture process zone (FPZ) length c_f directly from peak loads of notched beams.
Ignoring size scaling when moving from laboratory specimens to deep civil members introduces substantial unconservative error in unreinforced or lightly reinforced shear zones. Under our illustrative calibration (B f'_t = 4.20 MPa, transitional size D_0 = 220.0 mm, effective modulus E' = 34.0 GPa, g(α_0) = 1.12, g'(α_0) = 3.80), a 100 mm laboratory beam carries σ_N = 3.482 MPa (82.9% of B f'_t), a 400 mm beam drops to 2.502 MPa (59.6%), and a 2,000 mm full-scale girder falls to 1.322 MPa (31.5% of B f'_t, brittleness number β_B = 9.091). Extrapolating the small-scale plastic limit 4.20 MPa directly to D = 2,000 mm overestimates nominal fracture capacity by a factor of 3.177× in the model.
Every enduring equation begins as a human question—an act of patient curiosity by investigators who refused to accept an opaque boundary as the final word. Tracing the intellectual arc of Folio E.15 from its earliest formulation in 1921 (Alan Arnold Griffith derives the brittle energy-balance fracture criterion in solids, predicting nominal strength proportional to D^(−1/2) (Phil. Trans. R. Soc. Lond. A, DOI 10.1098/rsta.1921.0006[Scite ↗]).) to its modern resolution in 2024 (Qin, Lin, and Guo combine large-scale dam-concrete fracture tests with mesoscale aggregate simulation to examine aggregate-size effects on size-effect transition (Theoretical and Applied Fracture Mechanics, DOI 10.1016/j.tafmec.2024.104649[Scite ↗]).) reveals why un-coupled classical approximations repeatedly stalled at a hard analytical barrier. Whenever investigators attempted to treat the governing relation σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0) as a purely local or linearized perturbation, higher-order coupling terms across the kernel triad (Griffith LEFM (1921) · Hillerborg Fictitious Crack (1976) · Bažant Size Effect Law (1984, 1990)) amplified truncation error rather than damping it. What appeared for decades to be an intractable computational or experimental pathology was, in reality, a structural phase boundary embedded in the operator domain itself.
Resolving that impasse required shifting from ad-hoc empirical curve fitting to a rigorous, multi-stage operator formulation anchored in Model values (notched beam D = 400.0 mm, D_0 = 220.0 mm): β_B = 1.818 · σ_N = 2.502 MPa (59.6% of B f'_t) · s = −0.323 · G_f = 127.84 N/m · c_f = 64.84 mm (drops to σ_N = 1.322 MPa at D = 2000 mm). Specifically, the system’s trajectory is governed by control parameter P_1 (Structural Depth (D)) spanning the admissible interval [50.0, 2400.0] with step resolution Δ = 50.0 and reference operating point 400.0 mm; control parameter P_2 (Transitional Size (D_0)) spanning the admissible interval [80.0, 500.0] with step resolution Δ = 10.0 and reference operating point 220.0 mm. Within this state space, any valid proof or physical design must simultaneously satisfy local conservation laws, global boundary conditions, and strict asymptotic scaling—setting the stage for the four-chapter formal derivation in Act II.
"The aggregate-bridged fracture process zone does not grow with the bridge: as structural depth D outpaces transitional size D_0, nominal strength crosses smoothly from plastic yield toward Griffith D^(−1/2) brittleness."
§ I.2 · Historical Turning Points
Year
Milestone
1921
Alan Arnold Griffith derives the brittle energy-balance fracture criterion in solids, predicting nominal strength proportional to D^(−1/2) (Phil. Trans. R. Soc. Lond. A, DOI 10.1098/rsta.1921.0006[Scite ↗]).
1976
Arne Hillerborg, Mikael Modéer, and Per-Erik Petersson introduce the fictitious crack model with cohesive softening and characteristic length l_ch = E' G_f / (f'_t)^2 (Cement and Concrete Research, DOI 10.1016/0008-8846(76)90007-7[Scite ↗]).
1984
Zdeněk P. Bažant derives the Type II Size Effect Law σ_N = B f'_t / √(1 + D / D_0) by asymptotic matching of crack-band energy release and plastic limit (Journal of Engineering Mechanics, DOI 10.1061/(ASCE)0733-9399(1984)110:4(518)[Scite ↗]).
1990
Bažant and Mohammad T. Kazemi formulate linear regression of 1 / σ_N^2 vs. D to extract initial fracture energy G_f, FPZ length c_f, and brittleness number β_B (International Journal of Fracture, DOI 10.1007/BF00047063[Scite ↗]).
2009
Bažant and Qiang Yu generalize the Universal Size Effect Law across Type II notched and Type I unnotched quasi-brittle structures (Journal of Engineering Mechanics, DOI 10.1061/(ASCE)0733-9399(2009)135:2(78)[Scite ↗]).
2024
Qin, Lin, and Guo combine large-scale dam-concrete fracture tests with mesoscale aggregate simulation to examine aggregate-size effects on size-effect transition (Theoretical and Applied Fracture Mechanics, DOI 10.1016/j.tafmec.2024.104649[Scite ↗]).
Act II — Cross-Field Intuition: Perforated Paper, Aggregate Bridges & the Brittleness Number
Everyday Analogy & Interactive Controls Primer
Everyday Analogy: Compare tearing a small notched strip of heavy woven cardboard against tearing a wide poster board made of the same card stock. Along the notch tip, loose paper fibers fray and bridge across a finger-width zone about 20 mm wide. On a 30 mm narrow strip, that frayed zone spans nearly the whole remaining ligament, so you feel the strip pull evenly before parting. On a 1,000 mm wide sheet, the same 20 mm frayed zone sits like a tiny pinprick at the notch tip while elastic tension across the broad sheet concentrates energy right into that tip, unzipping the sheet at far lower average stress. This analogy stops where three-dimensional coarse-aggregate interlock and compressive shear friction replace pure tensile fiber tearing.
How the Two Sliders Work in Plain Words: Our interactive fracture laboratory controls two geometric and material scales from the Bažant–Kazemi model. The first slider is Structural Depth (D, from 50 to 2,400 mm), representing the height of a notched concrete beam tested in geometric proportion. Dragging D upward moves the specimen rightward along the size-effect curve, driving brittleness number β_B upward and dropping nominal strength σ_N toward the −1/2 elastic fracture slope. The second slider is Transitional Size (D_0, from 80 to 500 mm), which reflects how large the aggregate-bridged fracture process zone is relative to specimen geometry; raising D_0 expands fracture energy G_f and process-zone length c_f, lifting nominal strength across medium depths.
1 · EVERYDAY ANALOGY (E.15)
Frayed Process Zone vs. Structural Depth
Fixed process-zone length c_f shrinks relative to girder depth D as structures scale up
Slider 1: Structural Depth
Slider 2: Transitional Size
➜
2 · TWO COMPETING FORCES
▲ Structural Depth (D)
Raising D increases elastic energy stored per unit advance, lowering nominal stress σ_N
▼ Transitional Size (D_0)
Larger D_0 reflects wider aggregate bridging c_f and higher initial fracture energy G_f
➜
3 · CRITICAL TIPPING POINT
Brittleness Transition (β_B = D / D_0)
✓ STABLE / NOMINAL REGIME
Quasi-plastic small scale: β_B <= 0.15 keeps σ_N close to plastic intercept B f'_t
Plate E.15-D · Visual Intuition Bridge: Before diving into the formal equations, follow how the everyday physical analogy (left) sets two competing mechanisms in tension (center) around a sharp tipping point (right) that you can test directly with the two sliders in Act III.
In Bažant's (1984) energy-release balance, advancing a notch through a quasi-brittle beam releases strain energy from a band of width proportional to aggregate-controlled FPZ length c_f as well as from the outer elastic volume proportional to D. Combining both terms yields σ_N(D) = B f'_t / √(1 + D / D_0), where brittleness number β_B = D / D_0 measures structural size relative to the material-geometry crossover scale D_0. Taking the log–log derivative gives local slope s = d ln σ_N / d ln D = −β_B / [2(1 + β_B)], moving smoothly from 0 in the plastic limit (β_B → 0) to −0.5 in Griffith LEFM (β_B → ∞). Notice the calibration boundary: holding B f'_t = 4.20 MPa, E' = 34.0 GPa, f'_t = 3.20 MPa, g(α_0) = 1.12, and g'(α_0) = 3.80 fixed while varying D_0 scales initial fracture energy G_f = (B f'_t)^2 D_0 g(α_0) / E', process-zone length c_f = D_0 g(α_0) / g'(α_0), and Hillerborg characteristic length l_ch = E' G_f / (f'_t)^2 linearly with D_0. Live parameter coupling: Structural Depth = 400.0 mm under governing law
— in plain words: nominal concrete tensile strength declines with member size relative to a transition scale set by fracture energy and the finite fracture process zone.
Bažant and Kazemi (1990) turned this scaling relation into a direct laboratory extraction method. Squaring and inverting σ_N(D) gives Y = 1 / σ_N^2 = C D + A, where A = 1 / (B f'_t)^2 and C = 1 / [(B f'_t)^2 D_0]. Fitting five notched beams across D ∈ {100, 200, 400, 800, 1600} mm recovers B f'_t = 4.20 MPa and D_0 = 220.0 mm directly from regression slope C and intercept A, yielding initial fracture energy G_f = 127.84 N/m (note unit identity: MPa^2 · mm / GPa = N/m), effective FPZ length c_f = 64.84 mm, and Hillerborg l_ch = 424.5 mm. By contrast, replacing (1 + D / D_0) with 1 assumes scale-invariant plastic strength, leaving slope s = 0 and inflating a D = 2,000 mm girder's modeled capacity from 1.322 MPa to 4.200 MPa (a 3.177× unconservative defect).
σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0)
Kernels: Griffith LEFM (1921) · Hillerborg Fictitious Crack (1976) · Bažant Size Effect Law (1984, 1990) · Benchmarks: Model values (notched beam D = 400.0 mm, D_0 = 220.0 mm): β_B = 1.818 · σ_N = 2.502 MPa (59.6% of B f'_t) · s = −0.323 · G_f = 127.84 N/m · c_f = 64.84 mm (drops to σ_N = 1.322 MPa at D = 2000 mm) · Primary Anchor:DOI 10.1061/(ASCE)0733-9399(1984)110:4(518)
To elevate Folio E.15 (Quasi-Brittle Concrete Fracture, Bažant Size Effect Law & Hillerborg Process-Zone Scaling) from a qualitative summary to an executable mathematical and physical treatise, we first define the exact state-space manifold on which the operator σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0) acts. Let the system state be parameterized by control parameter P_1 (Structural Depth (D)) spanning the admissible interval [50.0, 2400.0] with step resolution Δ = 50.0 and reference operating point 400.0 mm; control parameter P_2 (Transitional Size (D_0)) spanning the admissible interval [80.0, 500.0] with step resolution Δ = 10.0 and reference operating point 220.0 mm. Over this bounded domain, the coupled kernels (Griffith LEFM (1921) · Hillerborg Fictitious Crack (1976) · Bažant Size Effect Law (1984, 1990)) map every admissible input configuration to a unique, deterministic equilibrium or deductive fixed point recomputed by skills/engineering/e15/verify_e15_bazant_size_effect.py.
Crucially, well-posedness across the Model values (notched beam D = 400.0 mm, D_0 = 220.0 mm): β_B = 1.818 · σ_N = 2.502 MPa (59.6% of B f'_t) · s = −0.323 · G_f = 127.84 N/m · c_f = 64.84 mm (drops to σ_N = 1.322 MPa at D = 2000 mm) regime requires that the governing operator preserve dimensional homogeneity, non-negativity of physical energy/entropy functionals, and strict monotony along the primary reaction or proof coordinate. Whenever a simplified model omits one of the coupled terms in σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0), the resulting approximation violates boundary compatibility and diverges from the primary peer-reviewed evidence (Scite Smart Citation Index entry for Bažant 1984, "Size Effect in Blunt Fracture: Concrete, Rock, Metal" (Journal of Engineering Mechanics, DOI 10.1061/(ASCE)0733-9399(1984)110:4(518)), fetched 2026-11-21: 1,772 citing records (35 supporting, 707 mentioning, 1 contrasting) and no retraction notice. These counts describe that foundational paper, not this folio.).
Rather than treating σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0) as an opaque black-box formula, we decompose the proof and physical mechanism of Folio E.15 into four clear, verifiable stages. True scientific tools do not ask for blind trust; they invite inspection. Each stage represents a rigorous transformation of the state vector—corresponding one-to-one with the 4-stage interactive stepper in Act III and the standalone verifier in skills/engineering/e15/verify_e15_bazant_size_effect.py:
Stage 1 Derivation & State Transition
Formal Stage Mechanism: Stage 1 (From Griffith LEFM to Hillerborg's Fictitious Crack Zone): Griffith (1921, DOI 10.1098/rsta.1921.0006[Scite ↗]) showed that a sharp crack in a brittle solid grows when stored elastic energy release matches surface energy, scaling nominal strength as D^(−1/2). Concrete is not ideally brittle: ahead of a visible notch, microcracking and aggregate bridging form a finite Fracture Process Zone (FPZ). Hillerborg, Modéer, and Petersson (1976, DOI 10.1016/0008-8846(76)90007-7[Scite ↗]) modeled this softening zone via tensile strength f'_t, initial fracture energy G_f, and characteristic length l_ch = E' G_f / (f'_t)^2 (424.5 mm at E' = 34.0 GPa, f'_t = 3.20 MPa, G_f = 127.84 N/m).
Operator Coupling & Invariant Closure: At Stage 1 of the Folio E.15 derivation chain, the intermediate state maps directly onto the governing law σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0) under benchmark regime Model values (notched beam D = 400.0 mm, D_0 = 220.0 mm): β_B = 1.818 · σ_N = 2.502 MPa (59.6% of B f'_t) · s = −0.323 · G_f = 127.84 N/m · c_f = 64.84 mm (drops to σ_N = 1.322 MPa at D = 2000 mm). To ensure that deductive or physical flux is conserved without unverified hand-waving as the system advances from Stage 1 toward terminal convergence, the transition operator enforces the companion verification constraint: Enforce strictly positive finite parameters D, D_0, B*f_t, E', f_t, g(alpha_0), and g'(alpha_0) inside geometrically similar notched Type II members (alpha_0 = a_0 / D > 0). Every numerical trajectory and geometric projection in Plate E.15-A and Plate E.15-B below evaluates this exact stage transfer function in real time.
Stage 2 Derivation & State Transition
Formal Stage Mechanism: Stage 2 (Bažant Type II Size Effect Law & Brittleness Number β_B): For geometrically similar notched members (notch ratio α_0 = a_0 / D > 0), Bažant (1984, DOI 10.1061/(ASCE)0733-9399(1984)110:4(518)[Scite ↗]) matched plastic yield at small D against LEFM at large D via σ_N(D) = B f'_t / √(1 + β_B), with brittleness number β_B = D / D_0. Using illustrative calibration B f'_t = 4.20 MPa and D_0 = 220.0 mm, a 100 mm laboratory beam reaches σ_N = 3.482 MPa (82.9% of B f'_t, β_B = 0.455), while a 400 mm beam drops to 2.502 MPa (59.6%, β_B = 1.818) and log–log slope s = −β_B / [2(1 + β_B)] steepens from −0.156 to −0.323.
Operator Coupling & Invariant Closure: At Stage 2 of the Folio E.15 derivation chain, the intermediate state maps directly onto the governing law σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0) under benchmark regime Model values (notched beam D = 400.0 mm, D_0 = 220.0 mm): β_B = 1.818 · σ_N = 2.502 MPa (59.6% of B f'_t) · s = −0.323 · G_f = 127.84 N/m · c_f = 64.84 mm (drops to σ_N = 1.322 MPa at D = 2000 mm). To ensure that deductive or physical flux is conserved without unverified hand-waving as the system advances from Stage 2 toward terminal convergence, the transition operator enforces the companion verification constraint: Compute nominal strength via Bazant Type II Size Effect Law sigma_N = B*f_t / sqrt(1 + D/D_0) with brittleness number beta_B = D / D_0 and log-log slope s = -beta_B / (2*(1 + beta_B)), avoiding scale-invariant plastic extrapolation. Every numerical trajectory and geometric projection in Plate E.15-A and Plate E.15-B below evaluates this exact stage transfer function in real time.
Stage 3 Derivation & State Transition
Formal Stage Mechanism: Stage 3 (Bažant–Kazemi Regression for G_f and Process-Zone Length c_f): Bažant and Kazemi (1990, DOI 10.1007/BF00047063[Scite ↗]) inverted the size-effect curve into a linear relation Y = 1 / σ_N^2 = C D + A, where G_f = (B f'_t)^2 D_0 g(α_0) / E' and effective FPZ length c_f = D_0 g(α_0) / g'(α_0). With LEFM geometry factors g(α_0) = 1.12 and g'(α_0) = 3.80 at D_0 = 220.0 mm, the model yields G_f = 127.84 N/m and c_f = 64.84 mm. Doubling D_0 to 440.0 mm (a tougher aggregate mix at fixed B f'_t) raises G_f to 255.68 N/m, c_f to 129.68 mm, and 400 mm beam nominal strength to 3.040 MPa.
Operator Coupling & Invariant Closure: At Stage 3 of the Folio E.15 derivation chain, the intermediate state maps directly onto the governing law σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0) under benchmark regime Model values (notched beam D = 400.0 mm, D_0 = 220.0 mm): β_B = 1.818 · σ_N = 2.502 MPa (59.6% of B f'_t) · s = −0.323 · G_f = 127.84 N/m · c_f = 64.84 mm (drops to σ_N = 1.322 MPa at D = 2000 mm). To ensure that deductive or physical flux is conserved without unverified hand-waving as the system advances from Stage 3 toward terminal convergence, the transition operator enforces the companion verification constraint: Check unit identity (MPa^2 * mm / GPa = N/m) when evaluating initial Mode I fracture energy G_f = (B*f_t)^2 * D_0 * g(alpha_0) / E', effective FPZ length c_f = D_0 * g(alpha_0) / g'(alpha_0), and Hillerborg characteristic length l_ch = E' * G_f / f_t^2 (mm). Every numerical trajectory and geometric projection in Plate E.15-A and Plate E.15-B below evaluates this exact stage transfer function in real time.
Stage 4 Derivation & State Transition
Formal Stage Mechanism: Stage 4 (Open Hypothesis, Tier T1–T2, and Falsification Condition): Hypothesis (Tier T1–T2): in geometrically similar notched concrete beams without distributed shear reinforcement, nominal failure stress declines along σ_N = B f'_t (1 + D / D_0)^(−1/2) toward Griffith D^(−1/2) scaling as structural depth grows; at D = 2000 mm (D_0 = 220 mm, β_B = 9.091), modeled σ_N falls to 1.322 MPa (31.5%, slope −0.450), whereas ignoring (1 + D / D_0) overpredicts capacity by 3.177× at 4.20 MPa. This Type II hypothesis is falsified in unnotched Type I beams governed by Weibull boundary-layer strength (Bažant & Yu 2009, DOI 10.1061/(ASCE)0733-9399(2009)135:2(78)[Scite ↗]), in heavily stirrup-confined or steel-fiber members that arrest localization, or where aggregate size d_a is comparable to D.
Operator Coupling & Invariant Closure: At Stage 4 of the Folio E.15 derivation chain, the intermediate state maps directly onto the governing law σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0) under benchmark regime Model values (notched beam D = 400.0 mm, D_0 = 220.0 mm): β_B = 1.818 · σ_N = 2.502 MPa (59.6% of B f'_t) · s = −0.323 · G_f = 127.84 N/m · c_f = 64.84 mm (drops to σ_N = 1.322 MPa at D = 2000 mm). To ensure that deductive or physical flux is conserved without unverified hand-waving as the system advances from Stage 4 toward terminal convergence, the transition operator enforces the companion verification constraint: Frame Type II size-effect scaling as a Tier T1-T2 structural screening hypothesis that stops at unnotched Type I beams, stirrup-confined or fiber-reinforced shear members, and code design checks. Every numerical trajectory and geometric projection in Plate E.15-A and Plate E.15-B below evaluates this exact stage transfer function in real time.
Every quantitative claim in Folio E.15 is tied to four falsification rules listed in bazant-size-effect-SKILL.md and executed by skills/engineering/e15/verify_e15_bazant_size_effect.py:
Invariant E.15-R1: Enforce strictly positive finite parameters D, D_0, B*f_t, E', f_t, g(alpha_0), and g'(alpha_0) inside geometrically similar notched Type II members (alpha_0 = a_0 / D > 0).
Recomputed offline by skills/engineering/e15/verify_e15_bazant_size_effect.py; primary anchor DOI 10.1061/(ASCE)0733-9399(1984)110:4(518).
Invariant E.15-R2: Compute nominal strength via Bazant Type II Size Effect Law sigma_N = B*f_t / sqrt(1 + D/D_0) with brittleness number beta_B = D / D_0 and log-log slope s = -beta_B / (2*(1 + beta_B)), avoiding scale-invariant plastic extrapolation.
Recomputed offline by skills/engineering/e15/verify_e15_bazant_size_effect.py; primary anchor DOI 10.1061/(ASCE)0733-9399(1984)110:4(518).
Invariant E.15-R3: Check unit identity (MPa^2 * mm / GPa = N/m) when evaluating initial Mode I fracture energy G_f = (B*f_t)^2 * D_0 * g(alpha_0) / E', effective FPZ length c_f = D_0 * g(alpha_0) / g'(alpha_0), and Hillerborg characteristic length l_ch = E' * G_f / f_t^2 (mm).
Recomputed offline by skills/engineering/e15/verify_e15_bazant_size_effect.py; primary anchor DOI 10.1061/(ASCE)0733-9399(1984)110:4(518).
Invariant E.15-R4: Frame Type II size-effect scaling as a Tier T1-T2 structural screening hypothesis that stops at unnotched Type I beams, stirrup-confined or fiber-reinforced shear members, and code design checks.
Recomputed offline by skills/engineering/e15/verify_e15_bazant_size_effect.py; primary anchor DOI 10.1061/(ASCE)0733-9399(1984)110:4(518).
Together, Invariants E.15-R1 through E.15-R4 close the epistemic loop between symbolic derivation and numerical execution. If a code edit violates these bounds, the verifier fails.
Primary Counterfactual Knockout (SIDENOTE E.15-A · INITIAL FRACTURE ENERGY G_f VS. TOTAL WORK OF FRACTURE G_F): Bažant and Kazemi (1990, DOI 10.1007/BF00047063[Scite ↗]) distinguish the initial fracture energy G_f—governed by the steep initial tangent of the cohesive softening curve and extracted from size-effect peak loads—from the larger total work of fracture G_F integrated under the entire softening tail. Peak-load structural size effect depends primarily on G_f and effective process-zone length c_f, whereas post-peak tail energy G_F governs late crack opening.
Secondary Coupling & Regime Boundary (SIDENOTE E.15-B · TYPE II NOTCHED BOUNDARIES & CONSTANT-B f'_t PARAMETERIZATION): This reduced 2-slider sweep holds B f'_t = 4.20 MPa, E' = 34.0 GPa, f'_t = 3.20 MPa, g(α_0) = 1.12, and g'(α_0) = 3.80 constant across D_0 ∈ [80, 500] mm, so G_f = (B f'_t)^2 D_0 g(α_0) / E', c_f, and l_ch all scale linearly with D_0 (comparing tougher versus more brittle mixes). The curve applies to notched Type II members (α_0 > 0); unnotched Type I beams retain a finite large-size asymptotic stress under Universal Size Effect Law (Bažant & Yu 2009, DOI 10.1061/(ASCE)0733-9399(2009)135:2(78)[Scite ↗]).
Mathematical & Physical Necessity of the Full Operator: Testing a theorem or physical law by knocking out its core hypothesis is one of the sharpest ways a human mind builds intuition. This counterfactual analysis shows why every coupling term in σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0) is indispensable: When the primary control parameter is dragged to its degenerate boundary in the Act III observatory below, the stabilizing restorative term vanishes, reproducing the classical collapse predicted by theory and illustrating that our solver is an interactive computational model rather than a static animation.
Act III — Interactive Laboratory & Worked Numerical Verification
§ III.1 · Three Guided Experiments to Try
Experiment 1 (Lab Beam vs. Full-Scale Girder at D_0 = 220 mm): Hold Transitional Size D_0 = 220 mm and sweep Structural Depth D from 100 mm up to 2,000 mm. Watch brittleness β_B climb from 0.455 to 9.091 while nominal strength σ_N falls from 3.482 MPa (82.9% of B f'_t) through 2.502 MPa at D = 400 mm down to 1.322 MPa (31.5% retention), with log–log slope steepening from −0.156 to −0.450.
Experiment 2 (Aggregate Toughness & Crossover D_0): Hold Structural Depth D = 400 mm and increase Transitional Size D_0 from 220 mm to 440 mm. Watch initial fracture energy G_f double from 127.84 N/m to 255.68 N/m and FPZ length c_f double from 64.84 mm to 129.68 mm, lifting modeled strength from 2.502 MPa (59.6%) to 3.040 MPa (72.4%) as the beam shifts back toward the ductile crossover.
Experiment 3 (Asymptotic Slope & 4-Lens Observatory): Drag D toward 2,400 mm at D_0 = 80 mm (β_B = 30.0) to inspect the LEFM brittle asymptote (σ_N = 0.754 MPa, slope s = −0.484 close to −0.500), and explore the 4-Lens Observatory tabs (3D Surface, Phase Portraits, Kirchhoff Ribbon, Polar Radar).
Stage 1 (From Griffith LEFM to Hillerborg's Fictitious Crack Zone): Griffith (1921, DOI 10.1098/rsta.1921.0006) showed that a sharp crack in a brittle solid grows when stored elastic energy release matches surface energy, scaling nominal strength as D^(−1/2). Concrete is not ideally brittle: ahead of a visible notch, microcracking and aggregate bridging form a finite Fracture Process Zone (FPZ). Hillerborg, Modéer, and Petersson (1976, DOI 10.1016/0008-8846(76)90007-7) modeled this softening zone via tensile strength f'_t, initial fracture energy G_f, and characteristic length l_ch = E' G_f / (f'_t)^2 (424.5 mm at E' = 34.0 GPa, f'_t = 3.20 MPa, G_f = 127.84 N/m).
§ III.2 · Worked Numerical Verification & Reference Telemetry Benchmark
To verify the interactive observatory above by hand or inside an independent computational notebook, we evaluate the governing law σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0) at the canonical benchmark configuration (Model values (notched beam D = 400.0 mm, D_0 = 220.0 mm): β_B = 1.818 · σ_N = 2.502 MPa (59.6% of B f'_t) · s = −0.323 · G_f = 127.84 N/m · c_f = 64.84 mm (drops to σ_N = 1.322 MPa at D = 2000 mm)). Substituting control parameter P_1 (Structural Depth (D)) spanning the admissible interval [50.0, 2400.0] with step resolution Δ = 50.0 and reference operating point 400.0 mm; control parameter P_2 (Transitional Size (D_0)) spanning the admissible interval [80.0, 500.0] with step resolution Δ = 10.0 and reference operating point 220.0 mm into the coupled Stage 1–4 equations yields the reference values recomputed by the verifier: Brittleness & Fracture Energy converges to β_B = 1.818 · G_f = 127.84 N/m (model); Nominal Strength & Retention converges to σ_N = 2.502 MPa (59.6% of B f'_t, model); Log–Log Slope & FPZ Length converges to s = −0.323 · c_f = 64.84 mm (model); Size-Effect Fracture Regime converges to QUASI-BRITTLE TRANSITION (0.15 < β_B <= 10, model).
Running python skills/engineering/e15/verify_e15_bazant_size_effect.py from the repository root recomputes these values, and its planted-defect mode must fail.
Act IV — Imagining Humanity's Future: Dam Safety, Mesoscale Digital Twins & Falsifiable Scaling
Large concrete dams, deep transfer girders, and nuclear containment shells sit well above the laboratory beam scale where standard cube and cylinder strengths are measured. Coupling closed-form Type II size-effect scaling with mesoscale aggregate experiments (Qin, Lin & Guo 2024, DOI 10.1016/j.tafmec.2024.104649[Scite ↗]) and offline regression verifiers allows structural engineers to keep size-dependent brittleness transparent alongside code provisions rather than extrapolating small-specimen stress linearly.
Under the Tier T1–T2 hypothesis stated here, geometrically similar notched concrete members without distributed shear reinforcement follow σ_N(D) = B f'_t (1 + D / D_0)^(−1/2), transitioning from plastic yield toward Griffith D^(−1/2) fracture as β_B = D / D_0 exceeds unity. This Type II hypothesis is explicitly falsified in unnotched Type I modulus-of-rupture beams where boundary-layer randomness yields a finite large-size asymptote (Bažant & Yu 2009, DOI 10.1061/(ASCE)0733-9399(2009)135:2(78)[Scite ↗]), in heavily stirrup-confined or fiber-bridged beams that prevent single-crack localization, or at miniature sizes D comparable to coarse-aggregate diameter d_a. Keeping a scale-invariant χ_size = 0 planted defect inside the verifier keeps plastic-extrapolation errors from passing automated screening.
Frontier discovery
Bažant Size Effect Law, Hillerborg Process Zones & Deep Concrete Girder Scaling
Why do small notched concrete test beams sustain higher nominal stress than two-meter bridge girders of the same batch? Coupling Hillerborg's fictitious crack model (1976) with Bažant's Type II Size Effect Law (1984, DOI 10.1061/(ASCE)0733-9399(1984)110:4(518)[Scite ↗]) tracks the shift from 3.482 MPa at D = 100 mm to 1.322 MPa at D = 2,000 mm (D_0 = 220 mm, G_f = 127.84 N/m).
§ IV.3 · Cross-Disciplinary Continuum & Systems Transfer
Structural & Mathematical Isomorphism (Continues E.02/E.09/E.11): One of the defining principles of Informatico.ai is that deep governing operators transcend disciplinary silos. The exact mathematical structure of Folio E.15 (σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0)) reappears across coupled multiscale systems: Continues E.02/E.09/E.11
Living Edition & Revision Provenance (REV 1.0): REV 1.0 (Published 2026-11-21): Volume VII Civil & Structural Engineering monograph continuing Folios E.02, E.09 & E.11 via Griffith energy balance (1921), Hillerborg fictitious crack softening (1976), Bažant Type II Size Effect Law (1984), Bažant–Kazemi G_f/c_f regression (1990), Universal Size Effect Law (2009), and dam-concrete mesoscale fracture experiments (2024). Verification note: all six primary DOIs in this folio were checked against Crossref and Scite on 2026-11-21 with zero retraction notices; all numerical outputs are recomputed offline by skills/engineering/e15/verify_e15_bazant_size_effect.py and represent illustrative closed-form fracture-scaling model values rather than laboratory test data. By pairing multi-chapter mathematical and physical derivations with interactive WebGL2/SVG observatories and downloadable SKILL.md companions, Folio E.15 equips engineers, mathematicians, physicists, and AI agents with a permanent, falsifiable building block for frontier discovery.
Act V — Sources
Griffith, A. A. (1921). VI. The phenomena of rupture and flow in solids. Philosophical Transactions of the Royal Society of London. Series A, 221, 163–198. DOI 10.1098/rsta.1921.0006[Scite ↗].
Hillerborg, A., Modéer, M., & Petersson, P.-E. (1976). Analysis of crack formation and crack growth in concrete by means of fracture mechanics and finite elements. Cement and Concrete Research, 6(6), 773–781. DOI 10.1016/0008-8846(76)90007-7[Scite ↗].
Bažant, Z. P., & Kazemi, M. T. (1990). Determination of fracture energy, process zone length and brittleness number from size effect, with application to rock and concrete. International Journal of Fracture, 44(2), 111–131. DOI 10.1007/BF00047063[Scite ↗].
Bažant, Z. P., & Yu, Q. (2009). Universal Size Effect Law and Effect of Crack Depth on Quasi-Brittle Structure Strength. Journal of Engineering Mechanics, 135(2), 78–84. DOI 10.1061/(ASCE)0733-9399(2009)135:2(78)[Scite ↗].
Qin, J., Lin, C., & Guo, J. (2024). Syncretic investigation on size effect in fracture behavior of dam concrete with physical experiment and mesoscale simulation. Theoretical and Applied Fracture Mechanics, 133, 104649. DOI 10.1016/j.tafmec.2024.104649[Scite ↗].
Nicholson, J. M., et al. (2021). scite: A smart citation index that displays the context of citations and classifies their intent using deep learning (https://scite.ai). Quantitative Science Studies, 2(3), 882–898. DOI 10.1162/qss_a_00146[Scite ↗].
Inspired by classic broadsheet crosswords: test your command of E.15’s governing laws and historical turning points. Switch to ES-MX in the masthead to unlock a completely independent Spanish crossword with its own grid and scientific vocabulary.
EN · INDEPENDENT ENGLISH EDITION (10×10)
0 / 58 Folios Sealed (EN: 0 · ES-MX: 0)
1 ACROSSSelect any cell or clue below to begin solving.
Across
Down
Select any cell or clue and type A–Z. Space toggles Across/Down; progress auto-saves to localStorage.
Scite Smart Citation Index entry for Bažant 1984, "Size Effect in Blunt Fracture: Concrete, Rock, Metal" (Journal of Engineering Mechanics, DOI 10.1061/(ASCE)0733-9399(1984)110:4(518)), fetched 2026-11-21: 1,772 citing records (35 supporting, 707 mentioning, 1 contrasting) and no retraction notice. These counts describe that foundational paper, not this folio.
Give any AI agent or engineering pipeline the governing equations of Folio E.15: a portable SKILL.md, a zero-dependency Python verifier (verify_e15_bazant_size_effect.py), or the live telemetry as JSON.
Show the SKILL.md source
---
name: bazant-size-effect
description: AI-agnostic civil structural fracture skill for Bazant Type II Size Effect Law, Hillerborg fictitious crack length l_ch, and Bazant-Kazemi extraction of fracture energy G_f and process-zone length c_f.
license: MIT
compatibility: Claude Code, GitHub Copilot, Cursor, Google Antigravity, OpenAI Codex, Ollama (Qwen 3.8 / Gemma 4)
---
# Quasi-Brittle Concrete Fracture, Bažant Size Effect Law & Hillerborg Process-Zone Scaling (Folio E.15)
A plain-text companion to the essay at https://informatico.ai/engineering/e15/ (`E.15 · Bažant Size Effect & Concrete Fracture · REV 1.0`, `REV 1.0`, redated `2026-11-21`).
## The governing relation
`σ_N(D) = B f'_t / √(1 + D / D_0) · β_B = D / D_0 · G_f = (B f'_t)² D_0 g(α_0) / E' · c_f = D_0 g(α_0) / g'(α_0)`
## Rules the essay derives
1. Enforce strictly positive finite parameters D, D_0, B*f_t, E', f_t, g(alpha_0), and g'(alpha_0) inside geometrically similar notched Type II members (alpha_0 = a_0 / D > 0).
2. Compute nominal strength via Bazant Type II Size Effect Law sigma_N = B*f_t / sqrt(1 + D/D_0) with brittleness number beta_B = D / D_0 and log-log slope s = -beta_B / (2*(1 + beta_B)), avoiding scale-invariant plastic extrapolation.
3. Check unit identity (MPa^2 * mm / GPa = N/m) when evaluating initial Mode I fracture energy G_f = (B*f_t)^2 * D_0 * g(alpha_0) / E', effective FPZ length c_f = D_0 * g(alpha_0) / g'(alpha_0), and Hillerborg characteristic length l_ch = E' * G_f / f_t^2 (mm).
4. Frame Type II size-effect scaling as a Tier T1-T2 structural screening hypothesis that stops at unnotched Type I beams, stirrup-confined or fiber-reinforced shear members, and code design checks.
## How it works, in four stages
- Stage 1 (From Griffith LEFM to Hillerborg's Fictitious Crack Zone): Griffith (1921, DOI 10.1098/rsta.1921.0006) showed that a sharp crack in a brittle solid grows when stored elastic energy release matches surface energy, scaling nominal strength as D^(−1/2). Concrete is not ideally brittle: ahead of a visible notch, microcracking and aggregate bridging form a finite Fracture Process Zone (FPZ). Hillerborg, Modéer, and Petersson (1976, DOI 10.1016/0008-8846(76)90007-7) modeled this softening zone via tensile strength f'_t, initial fracture energy G_f, and characteristic length l_ch = E' G_f / (f'_t)^2 (424.5 mm at E' = 34.0 GPa, f'_t = 3.20 MPa, G_f = 127.84 N/m).
- Stage 2 (Bažant Type II Size Effect Law & Brittleness Number β_B): For geometrically similar notched members (notch ratio α_0 = a_0 / D > 0), Bažant (1984, DOI 10.1061/(ASCE)0733-9399(1984)110:4(518)) matched plastic yield at small D against LEFM at large D via σ_N(D) = B f'_t / √(1 + β_B), with brittleness number β_B = D / D_0. Using illustrative calibration B f'_t = 4.20 MPa and D_0 = 220.0 mm, a 100 mm laboratory beam reaches σ_N = 3.482 MPa (82.9% of B f'_t, β_B = 0.455), while a 400 mm beam drops to 2.502 MPa (59.6%, β_B = 1.818) and log–log slope s = −β_B / [2(1 + β_B)] steepens from −0.156 to −0.323.
- Stage 3 (Bažant–Kazemi Regression for G_f and Process-Zone Length c_f): Bažant and Kazemi (1990, DOI 10.1007/BF00047063) inverted the size-effect curve into a linear relation Y = 1 / σ_N^2 = C D + A, where G_f = (B f'_t)^2 D_0 g(α_0) / E' and effective FPZ length c_f = D_0 g(α_0) / g'(α_0). With LEFM geometry factors g(α_0) = 1.12 and g'(α_0) = 3.80 at D_0 = 220.0 mm, the model yields G_f = 127.84 N/m and c_f = 64.84 mm. Doubling D_0 to 440.0 mm (a tougher aggregate mix at fixed B f'_t) raises G_f to 255.68 N/m, c_f to 129.68 mm, and 400 mm beam nominal strength to 3.040 MPa.
- Stage 4 (Open Hypothesis, Tier T1–T2, and Falsification Condition): Hypothesis (Tier T1–T2): in geometrically similar notched concrete beams without distributed shear reinforcement, nominal failure stress declines along σ_N = B f'_t (1 + D / D_0)^(−1/2) toward Griffith D^(−1/2) scaling as structural depth grows; at D = 2000 mm (D_0 = 220 mm, β_B = 9.091), modeled σ_N falls to 1.322 MPa (31.5%, slope −0.450), whereas ignoring (1 + D / D_0) overpredicts capacity by 3.177× at 4.20 MPa. This Type II hypothesis is falsified in unnotched Type I beams governed by Weibull boundary-layer strength (Bažant & Yu 2009, DOI 10.1061/(ASCE)0733-9399(2009)135:2(78)), in heavily stirrup-confined or steel-fiber members that arrest localization, or where aggregate size d_a is comparable to D.
## Reference values stated in the essay
- **Brittleness & Fracture Energy**: `β_B = 1.818 · G_f = 127.84 N/m (model)`
- **Nominal Strength & Retention**: `σ_N = 2.502 MPa (59.6% of B f'_t, model)`
- **Log–Log Slope & FPZ Length**: `s = −0.323 · c_f = 64.84 mm (model)`
- **Size-Effect Fracture Regime**: `QUASI-BRITTLE TRANSITION (0.15 < β_B <= 10, model)`
## Check it yourself
This skill ships a verifier that recomputes its values. Its planted-defect mode must fail:
```
python skills/engineering/e15/verify_e15_bazant_size_effect.py
python skills/engineering/e15/verify_e15_bazant_size_effect.py --planted-defect
```
## Primary source
- https://doi.org/10.1061/(ASCE)0733-9399(1984)110:4(518) (Scite report: https://scite.ai/reports/10.1061/(ASCE)0733-9399(1984)110:4(518))
- What the essay compares against: Model values (notched beam D = 400.0 mm, D_0 = 220.0 mm): β_B = 1.818 · σ_N = 2.502 MPa (59.6% of B f'_t) · s = −0.323 · G_f = 127.84 N/m · c_f = 64.84 mm (drops to σ_N = 1.322 MPa at D = 2000 mm)
## Recent research context
- **Bažant Size Effect Law, Hillerborg Process Zones & Deep Concrete Girder Scaling**: Why do small notched concrete test beams sustain higher nominal stress than two-meter bridge girders of the same batch? Coupling Hillerborg's fictitious crack model (1976) with Bažant's Type II Size Effect Law (1984, DOI 10.1061/(ASCE)0733-9399(1984)110:4(518)) tracks the shift from 3.482 MPa at D = 100 mm to 1.322 MPa at D = 2,000 mm (D_0 = 220 mm, G_f = 127.84 N/m).
#!/usr/bin/env python3
"""Deterministic verifier for Folio E.15: Bažant Size Effect Law, Hillerborg Fictitious Crack Model & Concrete Brittleness Scaling.
Governing relations (Bažant 1984, DOI 10.1061/(ASCE)0733-9399(1984)110:4(518);
Bažant & Kazemi 1990, DOI 10.1007/BF00047063; Hillerborg, Modéer & Petersson 1976,
DOI 10.1016/0008-8846(76)90007-7):
- Geometrically similar notched Type II concrete members (notch ratio alpha_0 = a_0 / D > 0,
dimensionless LEFM energy release g(alpha_0) > 0, g'(alpha_0) > 0):
beta_B = D / D_0 (dimensionless brittleness number)
sigma_N(D) = B * f'_t / sqrt(1 + beta_B) [MPa]
s(D) = d ln(sigma_N) / d ln(D) = -beta_B / (2*(1 + beta_B))
- Initial Mode I fracture energy and effective fracture process zone (FPZ) length:
G_f = (B * f'_t)^2 * D_0 * g(alpha_0) / E' [N/m, with MPa^2 * mm / GPa = N/m]
c_f = D_0 * g(alpha_0) / g'(alpha_0) [mm]
l_ch = E' * G_f / (f'_t)^2 [mm, with GPa * (N/m) / MPa^2 = mm]
Model scope & caveats:
- Applies strictly to geometrically similar Type II notched structures (alpha_0 > 0) where
macrocrack localization from a pre-existing notch or stress concentrator governs failure.
- Varying transitional size D_0 while holding B*f'_t, E', f'_t, g(alpha_0), and g'(alpha_0) fixed
scales G_f, c_f, and l_ch linearly with D_0 (comparing tougher vs. more brittle concrete mixes
at constant small-scale plastic strength B*f'_t).
- Does not cover unnotched Type I modulus-of-rupture beams (which follow Type I Weibull-energetic
scaling with a finite large-size asymptotic strength), heavily stirrup-confined shear members,
or ultra-high-strength fiber-reinforced composites.
Planted-defect mode (`--planted-defect`):
Drops the size-effect denominator (1 + D / D_0), extrapolating the scale-invariant small-specimen
plastic strength sigma_N = B * f'_t = 4.20 MPa across a full-scale D = 2000 mm girder (where
the Bažant Type II model gives 1.322 MPa, a 3.177x unsafe overprediction).
"""
from __future__ import annotations
import argparse
import json
import math
import sys
from typing import Any
def evaluate_size_effect(
structural_depth_d_mm: float = 400.0,
transitional_size_d0_mm: float = 220.0,
small_scale_strength_bft_mpa: float = 4.20,
effective_modulus_ep_gpa: float = 34.0,
tensile_strength_ft_mpa: float = 3.20,
lefm_g_alpha0: float = 1.12,
lefm_gp_alpha0: float = 3.80,
planted_defect: bool = False,
) -> dict[str, Any]:
"""Evaluate Bažant Type II Size Effect Law and Hillerborg fracture parameters."""
params = (
structural_depth_d_mm,
transitional_size_d0_mm,
small_scale_strength_bft_mpa,
effective_modulus_ep_gpa,
tensile_strength_ft_mpa,
lefm_g_alpha0,
lefm_gp_alpha0,
)
if not all(math.isfinite(v) for v in params):
raise ValueError("All fracture scaling parameters must be finite numbers")
if any(v <= 0.0 for v in params):
raise ValueError("D, D_0, B*f'_t, E', f'_t, g(alpha_0), and g'(alpha_0) must be strictly positive")
brittleness_beta_b = structural_depth_d_mm / transitional_size_d0_mm
effective_beta = 0.0 if planted_defect else brittleness_beta_b
retention_ratio = 1.0 / math.sqrt(1.0 + effective_beta)
nominal_strength_mpa = small_scale_strength_bft_mpa * retention_ratio
log_log_slope = -effective_beta / (2.0 * (1.0 + effective_beta))
# Unit identity: (MPa^2 * mm) / GPa = ((1e6 N/m^2)^2 * 1e-3 m) / (1e9 N/m^2) = 1 N/m
fracture_energy_gf_n_per_m = (
(small_scale_strength_bft_mpa ** 2) * transitional_size_d0_mm * lefm_g_alpha0
) / effective_modulus_ep_gpa
fpz_length_cf_mm = transitional_size_d0_mm * lefm_g_alpha0 / lefm_gp_alpha0
# Unit identity: (GPa * N/m) / MPa^2 = 1e-3 m = 1 mm
hillerborg_lch_mm = (effective_modulus_ep_gpa * fracture_energy_gf_n_per_m) / (
tensile_strength_ft_mpa ** 2
)
if effective_beta <= 0.15:
regime = "QUASI-PLASTIC LIMIT (β_B <= 0.15, model)"
elif effective_beta <= 10.0:
regime = "QUASI-BRITTLE TRANSITION (0.15 < β_B <= 10, model)"
else:
regime = "LEFM BRITTLE ASYMPTOTE (β_B > 10, model)"
return {
"folio": "E.15",
"structural_depth_d_mm": round(structural_depth_d_mm, 1),
"transitional_size_d0_mm": round(transitional_size_d0_mm, 1),
"brittleness_beta_b": round(effective_beta, 3),
"nominal_strength_mpa": round(nominal_strength_mpa, 3),
"retention_pct": round(retention_ratio * 100.0, 1),
"log_log_slope": round(log_log_slope, 3),
"fracture_energy_gf_n_per_m": round(fracture_energy_gf_n_per_m, 2),
"fpz_length_cf_mm": round(fpz_length_cf_mm, 2),
"hillerborg_lch_mm": round(hillerborg_lch_mm, 1),
"regime": regime,
"exact_nominal_strength_mpa": nominal_strength_mpa,
"exact_log_log_slope": log_log_slope,
}
def linear_regression_bazant_kazemi(
depths_mm: list[float],
strengths_mpa: list[float],
) -> tuple[float, float]:
"""Recover B*f'_t and D_0 via Y = 1/sigma_N^2 = C*D + A (Bažant & Kazemi 1990)."""
n = len(depths_mm)
if n < 2 or n != len(strengths_mpa):
raise ValueError("Need >= 2 paired (D, sigma_N) measurements")
if not all(math.isfinite(d) and d > 0.0 for d in depths_mm):
raise ValueError("All structural depths D must be finite and strictly positive")
if not all(math.isfinite(s) and s > 0.0 for s in strengths_mpa):
raise ValueError("All nominal strengths sigma_N must be finite and strictly positive")
xs = depths_mm
ys = [1.0 / (s * s) for s in strengths_mpa]
mean_x = sum(xs) / n
mean_y = sum(ys) / n
sxx = sum((x - mean_x) ** 2 for x in xs)
if not math.isfinite(sxx) or sxx <= 0.0:
raise ValueError("Need >= 2 distinct structural depths D for regression")
sxy = sum((x - mean_x) * (y - mean_y) for x, y in zip(xs, ys))
slope_c = sxy / sxx
intercept_a = mean_y - slope_c * mean_x
if not (math.isfinite(slope_c) and math.isfinite(intercept_a)) or slope_c <= 0.0 or intercept_a <= 0.0:
raise ValueError("Regression slope C and intercept A must be finite and strictly positive")
bft_recovered = 1.0 / math.sqrt(intercept_a)
d0_recovered = intercept_a / slope_c
return bft_recovered, d0_recovered
def run_checks(planted_defect: bool = False) -> dict[str, Any]:
default_beam = evaluate_size_effect(
structural_depth_d_mm=400.0,
transitional_size_d0_mm=220.0,
planted_defect=planted_defect,
)
small_lab_beam = evaluate_size_effect(
structural_depth_d_mm=100.0,
transitional_size_d0_mm=220.0,
planted_defect=planted_defect,
)
full_scale_girder = evaluate_size_effect(
structural_depth_d_mm=2000.0,
transitional_size_d0_mm=220.0,
planted_defect=planted_defect,
)
tough_beam = evaluate_size_effect(
structural_depth_d_mm=400.0,
transitional_size_d0_mm=440.0,
planted_defect=planted_defect,
)
sample_depths = [100.0, 200.0, 400.0, 800.0, 1600.0]
sample_strengths = [
evaluate_size_effect(
structural_depth_d_mm=d,
transitional_size_d0_mm=220.0,
planted_defect=planted_defect,
)["exact_nominal_strength_mpa"]
for d in sample_depths
]
failures: list[str] = []
if not (small_lab_beam["exact_nominal_strength_mpa"] > default_beam["exact_nominal_strength_mpa"] > full_scale_girder["exact_nominal_strength_mpa"]):
failures.append("Nominal strength must strictly decrease as structural depth D grows from 100 mm to 2000 mm")
if full_scale_girder["exact_nominal_strength_mpa"] >= 1.50:
failures.append(
f"Full-scale D=2000 mm girder strength {full_scale_girder['nominal_strength_mpa']} MPa exceeds Type II size-effect bound (<1.50 MPa)"
)
if full_scale_girder["exact_log_log_slope"] > -0.40:
failures.append(
f"Full-scale D=2000 mm log-log slope {full_scale_girder['log_log_slope']} failed to approach LEFM -0.5 asymptote"
)
if abs(default_beam["fracture_energy_gf_n_per_m"] - 127.84) > 0.05:
failures.append(f"Unexpected G_f at D_0=220 mm: {default_beam['fracture_energy_gf_n_per_m']}")
if abs(default_beam["fpz_length_cf_mm"] - 64.84) > 0.05:
failures.append(f"Unexpected c_f at D_0=220 mm: {default_beam['fpz_length_cf_mm']}")
if abs(default_beam["hillerborg_lch_mm"] - 424.5) > 0.5:
failures.append(f"Unexpected l_ch at D_0=220 mm: {default_beam['hillerborg_lch_mm']}")
if tough_beam["exact_nominal_strength_mpa"] <= default_beam["exact_nominal_strength_mpa"]:
failures.append("Doubling D_0 (tougher aggregate/FPZ) must raise nominal strength at fixed D = 400 mm")
try:
bft_rec, d0_rec = linear_regression_bazant_kazemi(sample_depths, sample_strengths)
if abs(bft_rec - 4.20) > 1e-6 or abs(d0_rec - 220.0) > 1e-6:
failures.append(f"Bažant-Kazemi regression mismatch: B*f'_t={bft_rec}, D_0={d0_rec}")
except ValueError as exc:
failures.append(f"Bažant-Kazemi regression failed: {exc}")
# Negative domain checks: non-positive depth, duplicate depths, and non-positive/NaN strength must raise ValueError
rejected_invalid = False
try:
evaluate_size_effect(structural_depth_d_mm=0.0)
except ValueError:
rejected_invalid = True
if not rejected_invalid:
failures.append("Domain check failed to reject D = 0 mm")
for bad_label, bad_args in (
("duplicate D", ([400.0, 400.0], [2.5, 2.5])),
("zero strength", ([100.0, 400.0], [0.0, 2.5])),
("negative strength", ([100.0, 400.0], [-3.4, 2.5])),
("NaN strength", ([100.0, 400.0], [float("nan"), 2.5])),
):
try:
linear_regression_bazant_kazemi(*bad_args)
failures.append(f"Regression failed to reject {bad_label}")
except ValueError:
pass
status = "FAIL" if failures else "PASS"
return {
"status": status,
"folio": "E.15",
"planted_defect": planted_defect,
"default_beam_400mm": default_beam,
"small_lab_beam_100mm": small_lab_beam,
"full_scale_girder_2000mm": full_scale_girder,
"tough_beam_d0_440mm": tough_beam,
"overprediction_ratio_at_2000mm": round(4.20 / full_scale_girder["exact_nominal_strength_mpa"], 3),
"failures": failures,
}
def main(argv: list[str] | None = None) -> int:
parser = argparse.ArgumentParser(description="Verify Folio E.15 Bažant Size Effect Law & Hillerborg FPZ model.")
parser.add_argument("--planted-defect", action="store_true", help="Drop (1 + D/D_0) size scaling (must fail).")
args = parser.parse_args(argv)
result = run_checks(planted_defect=args.planted_defect)
print(json.dumps(result, indent=2, ensure_ascii=False))
return 0 if result["status"] == "PASS" else 1
if __name__ == "__main__":
raise SystemExit(main())
Edition history & reviewPublished 2026-11-21 · Updated 2026-11-21 (REV 1.0)
REV 1.0 (Published 2026-11-21): Volume VII Civil & Structural Engineering monograph continuing Folios E.02, E.09 & E.11 via Griffith energy balance (1921), Hillerborg fictitious crack softening (1976), Bažant Type II Size Effect Law (1984), Bažant–Kazemi G_f/c_f regression (1990), Universal Size Effect Law (2009), and dam-concrete mesoscale fracture experiments (2024).
Verification note: all six primary DOIs in this folio were checked against Crossref and Scite on 2026-11-21 with zero retraction notices; all numerical outputs are recomputed offline by skills/engineering/e15/verify_e15_bazant_size_effect.py and represent illustrative closed-form fracture-scaling model values rather than laboratory test data.